铁酸锌还原焙烧试验研究

EXPERIMENTAL STUDY ON REDUCTION ROASTING OF ZINC FERRITE

  • 推荐 CAJ下载
  • PDF下载
  • 不支持迅雷等下载工具,请取消加速工具后下载。

【作者】 解立群施哲胡汉

【Author】 XIE Li-qun SHI Zhe HU Han (Faculty of Metallurgy and Energy Engineering,Kunming University of Science and Technology,Kunming 650093,China)

【机构】 昆明理工大学冶金与能源工程学院

【摘要】 对锌焙砂进行还原焙烧,再对还原焙砂进行浸出。浸出温度70~80℃;pH值2~3;液固比6∶1;浸出时间2 h。对比试验得到最佳还原焙烧的温度900℃、焙烧时间60 min、粉煤配比1∶10。这时锌的浸出率达到90%左右,铁浸出率15%左右。再对浸出渣磁选,得到了铁精矿。

【Abstract】 Zinc calcine is reduction roasted and then the reducing calcine is leached.The leaching temperature is 70~80℃,pH value is 2~3,and leaching time is 2h.The comparing experiments show that the best reduction temperature is 900℃ and roasting time is 60min,with pulverized coal proportion as 1∶10.Under this condition,the zinc leaching rate can reach about 90% and the iron leaching rate can reach about 15%.The leaching slag is treated by magnetic separation,and iron concentrate is obtained.

  • 【文献出处】 矿冶 ,Mining and Metallurgy , 编辑部邮箱 ,2011年03期
  • 【分类号】TF813
  • 【被引频次】26
  • 【下载频次】185
节点文献中: