节点文献

VRLA电池枝晶短路的分析

An analysis of dendrite short circuit in VRLA batteries

  • 推荐 CAJ下载
  • PDF下载
  • 不支持迅雷等下载工具,请取消加速工具后下载。

【作者】 严军华朱江川李伟善

【Author】 YAN Jun-hua~(1,2), ZHU Jiang-chuan~2, LI Wei-shan~1(1. Department of Chemistry, South China Normal University, Guangzhou, Guangdong 510631, China; 2. B.B. Battery Co., Ltd., Raoping, Guangdong 515700, China)

【机构】 华南师范大学化学系美美电池有限公司华南师范大学化学系 广东广州 510631 美美电池有限公司广东饶平  51 570 0广东饶平 515700广东广州 510631

【摘要】 为了解阀控式铅酸(VRLA)电池在使用过程中发生枝晶短路的原因及机理,采用两种电池进行小电流深度过放电实验,并用扫描电子显微镜观察了电池隔板的形貌。结果表明:隔板较薄的电池容易产生枝晶短路。对VRLA电池枝晶短路产生的原因进行了分析。

【Abstract】 In order to obtain the cause and the mechanism of dendrite short circuit that took place in valve-regulated lead acid (VRLA) batteries, two kinds of batteries were taken for over-discharge experiment with small current and the morphologies of the separators in the batteries (before) and after over-discharge were observed by scan electron microscopy. The results indicated that the battery assembled by thinner separator was susceptible to dendrite short circuit. The reasons of dendrite short circuit in VRLA (batteries) were discussed.

【基金】 广东省自然科学基金资助项目(031533)
  • 【文献出处】 电池 ,Battery Bimonthly , 编辑部邮箱 ,2005年01期
  • 【分类号】TM912.1
  • 【被引频次】1
  • 【下载频次】158