节点文献

GCr15钢轴承套圈的失效分析

Failure Analysis on Bearing Ring Made of GCr15 Steel

  • 推荐 CAJ下载
  • PDF下载
  • 不支持迅雷等下载工具,请取消加速工具后下载。

【作者】 李宝银王慧董向红李忆莲李娟

【Author】 LI Bao-yin 1,WANG Hui 1,DONG Xiang-hong 1,LI Yi-lian 1,LI Juan 2 (1.Department of Materials Science and Engineering,Tianjin University,Tianjin 300072,China; 2.Tianjin 6443 Factory,Tianjin 300232,China)

【机构】 天津大学金属材料系!天津300072天津6443厂技校!天津300232

【摘要】 GCr1 5钢制造的轴承套圈 ,内径2 2 0mm ,高度H =1 57mm ,厚度b=1 2mm。在轧钢机上运转 1 4天 ,套圈表面辊道出现桔皮状条带 ,凹凸不平 ,影响正常工作。检验证明 ,原材料碳化物呈带状 ,热处理组织不合格 ,回火后出现粗大马氏体 ,导致套圈变形 ,圆度超标引起的摩擦过烧现象。

【Abstract】 A bearing ring which was made of GCr15 steel worked in the rolling machine.After 14 days working,the orange peel belt appeared on the roller bed.The test discovered that GCr15 steel contains belt carbides and the heat treatment process did not meet its requirement.The tempered martensite is coarse,so that there are much internal stress in the bearing ring which results in distortion of crystal lattice and the overrange of roundness,so it had been burn down in work.

【关键词】 轴承套圈失效分析等温淬火
【Key words】 bearing ringfailure analysisaustempering
  • 【文献出处】 金属热处理 ,HEAT TREATMENT OF METALS , 编辑部邮箱 ,2000年09期
  • 【分类号】TH133.3
  • 【被引频次】8
  • 【下载频次】233
节点文献中: