节点文献
炼油污水储罐的腐蚀与防护
Corrosion of Refinery Waste Water Tanks and Protection
【摘要】 锦州石化公司 3 0 0 0m3炼油污水储罐因Cl- ,NH3,CN- 和酚等腐蚀介质的影响 ,致使原环氧防腐蚀涂层失效并有 3 0 0多处点蚀穿孔。经试验 ,聚硫橡胶改性环氧树脂对上述介质有良好的耐蚀性 ,随后用环氧聚硫橡胶玻璃鳞片玻璃钢内衬对储罐进行了修复 ,经近 4年使用 ,效果良好
【Abstract】 On the 3000 m 3 refinery waste water tank in Jinzhou Petrochemical Company, the epoxy resin corrosion protection coating failed and more than 300 pittings were found due to the corrosion media of Cl -, NH 3 and CN -. The test demonstrated that the polysulfide-rubber-modified epoxy was highly resistant to the corrosion by above corrosive media. The tank was then repaired using FRP lining with polysulfide rubber glass scale and has been operating for four years without any problem ever since.
【关键词】 污水罐;
腐蚀;
聚硫橡胶改性环氧树脂;
玻璃鳞片;
玻璃钢;
衬里;
【Key words】 waste water tank; corrosion; polysulfide-rubber-modified epoxy; glass scale; FRP; lining;
【Key words】 waste water tank; corrosion; polysulfide-rubber-modified epoxy; glass scale; FRP; lining;
- 【文献出处】 石油化工腐蚀与防护 ,Petrochemical Corrosion and Protection , 编辑部邮箱 ,2002年04期
- 【分类号】TE988
- 【被引频次】2
- 【下载频次】106