节点文献
珠钢CSP薄板坯凝固层厚度研究
RESEARCH ON THE THICKNESS OF SOLIDIFIED SHELL OF CSP THIN SLAB
【摘要】 结合珠钢生产实际情况,采用射钉法来测定二冷区不同位置的凝固坯壳厚度,试验结果表明,4.8m/min拉速下铸坯液芯长度为4820mm,4.5m/min拉速下铸坯液芯为4490mm,两种拉速下连铸坯坯壳厚度的实际测量结果与凝固传热模型计算结果一致。整个凝固过程坯壳厚度生长符合平方根定律。
【Abstract】 The thickness of solidified shell of CSP thin slab located in different second cooling zones was determined by nailshooting in production The testing results indicated that the length of liquid core of thin slab is 4820 mm at a speed of 48 m/min, and 4490 mm at a speed of 45 m/min The testing results coincide very well with the simulation results of mathematical heat transfer model The growth of solidified shell accords with the square root rule in whole solidification process
【关键词】 CSP;
薄板坯连铸;
连铸坯坯壳;
射钉法;
【Key words】 CSP; thin slab continuous casting; solidification shell; nailshooting means;
【Key words】 CSP; thin slab continuous casting; solidification shell; nailshooting means;
- 【文献出处】 钢铁 ,Iron and Steel , 编辑部邮箱 ,2003年08期
- 【分类号】TF777
- 【被引频次】15
- 【下载频次】207