节点文献
影响Ly12铝合金锯齿流变诸因素的研究
Effect of Some Factors on the Serrated Flow in Ly12 Alloy
【摘要】 本文研究了应变速率,温度,自然时效时间,淬火后短期人工时效处理和预拉伸应变等因素对Ly12铝合金锯齿流变的影响。结果表明:淬火后短期人工时效处理,或延长淬火后室温停留时间,均有推迟锯齿流变产生的作用,而应变速率低于1.04×10-5秒-1,温度低于-55℃,高于90℃都不出现锯齿流变。
【Abstract】 The effects of temperature, rate of strain, time of natural aging, artificial aging for a short-term after quenching and pretensioning strain on the serrated flow in Lyl2 alloy were studied.It is shown that the serrated flow may be delayed by short-term artificial aging or prolonging the time of natural aging after quenching.The serrated flow doesn’t take place at the rate of strain below 1.04×10-5s-1, and at the temperature below -55℃ or above 90℃.
【关键词】 金属力学性质;
铝合金;
P—L效应;
锯齿流变;
【Key words】 mechanical properties; aluminium alloy; P-L effect; serrated flow;
【Key words】 mechanical properties; aluminium alloy; P-L effect; serrated flow;
- 【文献出处】 东北工学院学报 , 编辑部邮箱 ,1986年01期
- 【被引频次】1
- 【下载频次】68